What is flash curing, and how long should a flash be?

Published , by the PrintBlob team.

Flash curing is the brief heating of a freshly printed ink layer with a flash dryer, a radiant heater on the press, until it is dry to the touch but not fully cured, so another ink can be printed over it. Screen Printing Magazine says the technique has been routine in garment printing for more than 25 years, and that it is mostly used on dark garments: roughly two thirds of the colours in such a job are flashed.

It is the step between underbase and colours, and it is easy to get subtly wrong.

The target: dry, not done

A flash is not a mini cure. The goal is the least time and temperature that leave the surface dry and not tacky, because a hotter flash is not necessarily a faster one.

Setting What the sources give
Time three to five seconds is typical
Ink temperature about 125 to 250 °F, measured with a non-contact thermometer
Danger zone about 230 to 260 °F or more
Height of heater 1.5 to 2 inches above a t-shirt, doubled for hoodies and thick garments (Ryonet, for an underbase)
Check the surface is dry to the touch and not tacky

If the flashed layer is taken past the danger zone, it effectively cures, and the next ink cannot fuse to it. The print may then look fine and separate after a few washes. If it is under-flashed, the squeegee drags it as the next colour goes on.

Why order matters

Flashing makes wet-on-wet printing unnecessary. Screen Printing Magazine warns that printing wet-on-wet over a solid flashed underbase causes excess mottling. Ryonet adds that a slow printer should raise the heater slightly.

The fabric changes the setting

A garment of 100% cotton tolerates more heat than polyester, which can also release its dye if overheated. When you change shirts, check the flash with a temperature gun before you print the run, and write the settings down for the next order of the same blank. Screen Printing Magazine advises documenting the settings you establish.

Pair the flash with a real cure at the end of the line: the final dryer must bring the entire ink layer to the ink’s cure temperature, as set out in curing.

Sources