What is puff ink and how is it printed?

Published , by the PrintBlob team.

Puff ink is ink mixed with an additive full of tiny spherules that expand when heated, lifting the print into a soft, raised texture.

It is a way of selling a printed shirt on touch rather than picture, and it is easy to ruin with a dryer that runs too hot.

The recipe

ScreenPrinting.com’s guide to its FN-INK puff additive gives the working figures:

Item Figure
Additive 10 to 20 per cent by weight; above 20 per cent the ink can become unstable and flaky after washing
Mesh 86 to 110, with a slightly thicker stencil; 110 to 157 for thin-thread mesh; higher-tension screens strongly recommended
Stencil Any emulsion works, but high-solids emulsion builds the thickness in fewer coats; you should be able to feel the emulsion’s edge with a finger
Squeegee 60 durometer, or 70 if needed; a harder blade gives a thinner deposit and less puff
Printing Slightly more off-contact; a flood stroke helps, and two passes build more deposit
Activates Around 200 °F; full puff at 260 °F
Collapse Stable to about 280 to 290 °F; hotter, and the puff collapses

The bluntest line in the article is about the dryer: “Do not run the dryer hot and fast.” Use low heat and a slow belt speed.

Direct or over an underbase

  • Direct on the shirt. The shirt puckers, which makes the puff more visible, but the puff picks up the fabric texture and looks rougher.
  • Over an underbase. The puff looks smoother and less prominent. The underbase may still be curing as the puff activates, so cure more gently: see underbase.

What goes wrong

  • Premature puff. Too much flash heat activates the puff early, so it over-cures and collapses, and later colours are harder to print.
  • Weak puff. A hard squeegee, a thin deposit or too little additive.
  • Flaking. Additive over 20 per cent.
  • Brittle prints. An under-cured print is brittle and will not puff properly. A properly cured print is wash-stable, and a wash test gives the most reliable answer; a light abrasion test checks flaking.

For a shop

Puff is a screen-printing technique for repeat designs, not for a customer’s photo, and it takes more set-up than a flat print. Name the effect in the product description and show it with a close-up; a live preview on a flat mockup cannot show height. If a customer asks for it on an online-designed product, treat it as a finishing option you apply to flat shapes.

Sources